Abstract

A pavement sealing composition and method of application of the sealant to pavement to form a thin coating which protects the pavement, particularly asphalt from the harmful effects of oxidation, water, ice and snow as well as fluids spilled onto the pavement surface from automobiles and aircraft. Preferably, the coating is formed of a polymer based emulsion.

Claims (18)

1 . (canceled)

2 . (canceled)

3 . A method of applying a polymer emulsion onto a pavement surface comprising the steps of:

a) pouring a quantity of polymer emulsion concrete onto a pavement surface;

b) spreading said quantity of polymer emulsion into a layer of approximately 1/64 th to 1/32 nd of an inch in thickness;

c) allowing said polymer emulsion to dry on the pavement surface;

d) whereby, said polymer emulsion when dry forms a hard, durable seal over the pavement surface.

4 . A method of preparation of a polymer emulsion for sealing pavement comprising the steps of:

a) adding about 15 gallons of Rhoplex E-330 to a mixing vat;

b) set a disperser attached to said mixing vat at a high speed setting;

c) add approximately 32 ounces of Supersperse 100 and continue mixing for about 3 minutes;

d) adding at a measured rate about 25 pounds of titanium dioxide to the mixture and then mixing at high speed for about 45 minutes;

e) adding about 32 ounces of a defoaming agent to the mixture and then mixing at low speed for about 10 minutes;

f) adding about 35 gallons of Rhoplex E-330 to the mixture and mixing at low speed for about 10 minutes;

g) adding about 2 pounds of Rocima 63 to the mixture and mixing at low speed for about 10 minutes

h) adding about 25 gallons of water and mixing for a predetermined period of time;

i) adding about 2,800 pounds of Portland cement and sand and mixing for a predetermined period of time; and,

j) adding about 200 pounds of Unamin 2095 Granusil and mixing for about 3 minutes.

Assignments (1)