IP Library Granted Patent US 8,865,112
Granted Patent B2
US 8,865,112 · App. 13/498,032 · Granted Oct 21, 2014

Process and apparatus for multistage thermal treatment of rubber waste, in particular scrap tires

Inventors: Fikret Dülger (Vienna, AT); Niels Raeder (München, DE)
Assignee: Pyrolyx AG
C10B53/07C09C1/482C10B47/44B82Y30/00C10B7/10C10G1/10C01P2006/80C01P2004/64
View Patent ↗
Loading inventors, assignments & file history…
Monitor This Case
Get email alerts when status or documents change.
Order Certified Copies
Most orders are placed with the USPTO same day — all within 24 business hours.
Order via The Patent Place →
Pre-filled with this patent's details
Quick Facts
Patent No.
US 8,865,112
App. No.
13/498,032
Granted
Oct 21, 2014
Kind
B2
Abstract

A process for multistage thermal treatment of rubber waste, in particular scrap tires, is proposed. The process comprises several steps of transferring a product granulate of rubber waste into three different sequencing heating zones of a reactor ( 10 ). In the heating zones ( 11 a, 11 b, 11 c ) the product granulate is heated at a first temperature between 100° to 200° C., preferably 150° to 180° C., then at a second temperature between 200° to 350° C. and at a third temperature between 300° to 600° C. The temperature is maintained until such time that no further oil is emitted within the respective heating zone. As a final step, the product granulate is removed from the reactor ( 10 ) and the desirable solid materials are separated.

Claims (35)

1. Process for multistage thermal treatment of rubber waste to produce carbon black comprising the steps of:

transferring a product granulate of the rubber waste from a supply into a reactor;

heating the product granulate for a time period of between 2 to 4 hours at a first temperature between 100° to 200° C. in a first heating zone of the reactor until light oils emitting from the product granulate at temperatures between 100° to 200° C. are no longer emitted;

transferring the product granulate from the first heating zone to a second heating zone in the reactor;

heating the product granulate for a time period of between 2 to 4 hours at a second temperature between 200° to 300° C. in the second heating zone of the reactor until medium heavy oils emitting from the product granulate at temperatures between 200° to 300° C. are no longer emitted;

transferring the product granulate from the second heating zone to a third heating zone in the reactor;

heating the product granulate for a time period of between 2 to 4 hours at a third temperature between 300° to 600° C. in the third heating zone until heavy oils emitting from the product granulate at temperatures between 300° to 600° C. are no longer emitted; and

removing the product granulate from the reactor and separating the desirable solid materials, wherein each of the heating steps is carried out within a low pressure environment of about 20 to 50 mbar in each heating zone.

2. The process according to claim 1 in which the step of heating the product granulate at a first temperature includes heating the product granulate at the first temperature between 150° to 180° C., in the first heating zone of the reactor until light oils are no longer emitted.

3. Process for multistage thermal treatment of rubber waste to produce carbon black, comprising the steps of:

transferring a product granulate of the rubber waste from a supply into a reactor;

heating the product granulate for a time period of between 2 to 4 hours at a first temperature between 100° to 200° C. in a first heating zone of the reactor until light oils are no longer emitted;

transferring the product granulate from the first heating zone to a second heating zone in the reactor;

heating the product granulate for a time period of between 2 to 4 hours at a second temperature between 200° to 300° C. in the second heating zone of the reactor until medium heavy oils are no longer emitted;

transferring the product granulate from the second heating zone to a third heating zone in the reactor;

heating the product granulate for a time period of between 2 to 4 hours at a third temperature between 300° to 600° C. in the third heating zone until heavy oils are no longer emitted; and

removing the product granulate from the reactor and separating the desirable solid materials including carbon black, wherein each of the heating steps is carried out within a low pressure environment of about 20 to 50 mbar and wherein the carbon black recovered is refined at high temperatures for a time period of about 2 hours.

4. The process according to claim 1 wherein the product granulate is slowly moved within and through the reactor.

5. The process according to claim 4 , wherein the product is moved by means of a conveyor screw.

6. Process for multistage thermal treatment of rubber waste to produce carbon black, comprising the steps of:

transferring a product granulate of the rubber waste from a supply into a reactor;

heating the product granulate for a time period of between 2 to 4 hours at a first temperature between 100° to 200° C. in a first heating zone of the reactor until light oils are no longer emitted;

transferring the product granulate from the first heating zone to a second heating zone in the reactor;

heating the product granulate for a time period of between 2 to 4 hours at a second temperature between 200° to 300° C. in the second heating zone of the reactor until medium heavy oils are no longer emitted;

transferring the product granulate from the second heating zone to a third heating zone in the reactor;

heating the product granulate for a time period of between 2 to 4 hours at a third temperature between 300° to 600° C. in the third heating zone until heavy oils are no longer emitted; and

removing the product granulate from the reactor and separating the desirable solid materials including carbon black, wherein each of the heating steps is carried out within a low pressure environment of about 20 to 50 mbar and wherein the reactor is filled to about 60% of its volume.

7. Process for multistage thermal treatment of rubber waste to produce carbon black, comprising the steps of:

transferring a product granulate of the rubber waste from a supply into a reactor;

heating the product granulate for a time period of between 2 to 4 hours at a first temperature between 100° to 200° C. in a first heating zone of the reactor until light oils are no longer emitted;

transferring the product granulate from the first heating zone to a second heating zone in the reactor;

heating the product granulate for a time period of between 2 to 4 hours at a second temperature between 200° to 300° C. in the second heating zone of the reactor until medium heavy oils are no longer emitted;

transferring the product granulate from the second heating zone to a third heating zone in the reactor;

heating the product granulate for a time period of between 2 to 4 hours at a third temperature between 300° to 600° C. in the third heating zone until heavy oils are no longer emitted; and

removing the product granulate from the reactor and separating the desirable solid materials including carbon black, wherein each of the heating steps is carried out within a low pressure environment of about 20 to 50 mbar and wherein a cleaning step is carried out for about 2 hours at high temperatures without further product feeding.

Assignments (1)
CHANGE OF NAME Recorded Feb 24, 2013
From: SCUTUM CAPITAL AG
To: PYROLYX AG
Reel/Frame 029864/0043 →
Continuity (1)
Related Publication 20130064754A1 · Mar 14, 2013