IP Library › Granted Patent US 12,384,727
Granted Patent B2
US 12,384,727 · App. 17/851,269 · Granted Aug 12, 2025

Composite components and methods for preventing flow from infiltrated component during re-infiltration

Inventors: Juan P. Borja (Latham, NY); Daniel Gene Dunn (Guilderland, NY); Jared Hogg Weaver (Clifton Park, NY); Anant Achyut Setlur (Niskayuna, NY)
Assignee: General Electric Company
C04B37/003B32B18/00F01D5/282F01D25/005C04B2237/16C04B2237/38C04B2237/61C04B2237/84F05D2220/32F05D2230/20F05D2240/12F05D2240/30F05D2300/6033
View Patent ↗
Loading inventors, assignments & file history…
Monitor This Case
Get email alerts when status or documents change.
Order Certified Copies
Most orders are placed with the USPTO same day — all within 24 business hours.
Order via The Patent Place →
Pre-filled with this patent's details
Quick Facts
Patent No.
US 12,384,727
App. No.
17/851,269
Granted
Aug 12, 2025
Kind
B2
Abstract

A method for modifying a composite component may include positioning a barrier segment between an infiltrated segment of the composite component and a green segment to form an assembly; and initiating an infiltration process. The barrier segment may have a barrier segment permeability that is lower than a permeability of the infiltrated segment, a permeability of the green segment, or both. A composite component may include an infiltrated segment infiltrated with a molten material during a prior infiltration process; a green segment that is uninfiltrated; and a barrier segment having a microstructure different from the infiltrated segment, the green segment, or both. The microstructure of the barrier segment may be configured to slow a flow of material between the infiltrated segment and the green segment during a subsequent infiltration process.

Claims (42)

1. A method for modifying a composite component, comprising:

positioning a barrier segment between an infiltrated segment of the composite component and a green segment to form an assembly, wherein a particle size distribution varies from the barrier segment to the green segment; and

initiating an infiltration process,

wherein the barrier segment has a barrier segment permeability that is lower than an infiltrated segment permeability of the infiltrated segment, a green segment permeability of the green segment, or both the infiltrated segment permeability and the green segment permeability.

2. The method of claim 1 , wherein the composite component is a ceramic matrix composite (CMC) component, and wherein the infiltration process is a silicon infiltration process.

3. The method of claim 2 , wherein initiating the infiltration process comprises positioning a source of silicon in contact with at least the green segment.

4. The method of claim 3 , wherein initiating the infiltration process further comprises disposing the assembly and the source of silicon in a furnace and raising a temperature within the furnace above a melting point of silicon.

5. The method of claim 2 , wherein the silicon infiltration process is a melt-infiltration process.

6. The method of claim 1 , wherein the particle size distribution varies from smaller particles in the barrier segment to larger particles in the green segment.

7. The method of claim 1 , wherein the infiltrated segment was infiltrated prior to initiating the infiltration process such that initiating the infiltration process comprises initiating a second infiltration of the infiltrated segment.

8. The method of claim 1 , wherein the barrier segment permeability is one-half or less of the green segment permeability.

9. A method for modifying a ceramic matrix composite (CMC) component, comprising:

positioning a barrier segment between an infiltrated segment of the CMC component and a green segment, wherein a particle size distribution varies from the barrier segment to the green segment;

positioning a source of silicon in contact with the green segment; and

initiating a melt infiltration process,

wherein the barrier segment has a reactive permeability lower than a reactive permeability of the infiltrated segment, a reactive permeability of the green segment, or both the reactive permeability of the infiltrated segment and the reactive permeability of the green segment.

10. The method of claim 9 , wherein the melt infiltration process comprises positioning a source of silicon in contact with at least the green segment.

11. The method of claim 10 , wherein initiating the melt infiltration process is performed within a furnace by raising a temperature within the furnace above a melting point of silicon.

12. The method of claim 9 , wherein the particle size distribution varies from smaller particles in the barrier segment to larger particles in the green segment.

13. A method for modifying a composite component, comprising:

positioning a barrier segment between an infiltrated segment of the composite component and a green segment to form an assembly, wherein the green segment comprises the barrier segment; and

initiating an infiltration process,

wherein the barrier segment has a barrier segment permeability that is lower than an infiltrated segment permeability of the infiltrated segment, a green segment permeability of the green segment, or both the infiltrated segment permeability and the green segment permeability.

14. The method of claim 13 , wherein a particle size distribution varies from the barrier segment to the green segment.

15. The method of claim 13 , wherein the barrier segment defines an interface surface, the interface surface contacting the infiltrated segment.

16. A method for modifying a composite component, comprising:

positioning a barrier segment between an infiltrated segment of the composite component and a green segment to form an assembly; and

initiating an infiltration process,

wherein the barrier segment has a barrier segment permeability that is lower than an infiltrated segment permeability of the infiltrated segment, a green segment permeability of the green segment, or both the infiltrated segment permeability and the green segment permeability, and wherein the barrier segment permeability is a reactive permeability such that the barrier segment permeability is lower when the barrier segment reacts during the infiltration process.

17. The method of claim 16 , wherein the reactive permeability of the barrier segment is lower than a reactive permeability of the green segment.

18. A method for modifying a composite component, comprising:

identifying an area of unwanted material in an infiltrated segment;

removing the area of unwanted material;

thereafter, positioning a barrier segment between the infiltrated segment of the composite component and a green segment to form an assembly; and

initiating an infiltration process,

wherein the barrier segment has a barrier segment permeability that is lower than an infiltrated segment permeability of the infiltrated segment, a green segment permeability of the green segment, or both the infiltrated segment permeability and the green segment permeability.

19. A method for modifying a composite component, comprising:

forming a green segment from a first plurality of composite plies;

forming a barrier segment from a second plurality of composite plies;

positioning the barrier segment between an infiltrated segment of the composite component and the green segment to form an assembly; and

initiating an infiltration process,

wherein the barrier segment has a barrier segment permeability that is lower than an infiltrated segment permeability of the infiltrated segment, a green segment permeability of the green segment, or both the infiltrated segment permeability and the green segment permeability.

Assignments (1)
ASSIGNMENT OF ASSIGNOR'S INTEREST Recorded Jun 28, 2022
From: BORJA, JUAN P.; DUNN, DANIEL GENE; WEAVER, JARED HOGG; SETLUR, ANANT ACHYUT
To: GENERAL ELECTRIC COMPANY
Reel/Frame 060334/0243 →
Continuity (1)
Related Publication 20230416162A1 · Dec 28, 2023
References Cited (17)
US 6820334B2 · Kebbede et al. · 2004 [cited by applicant]
US 7966707B2 · Szela et al. · 2011 [cited by applicant]
US 9366140B2 · Chamberlain · 2016 [cited by applicant]
US 10150188B1 · Parolini et al. · 2018 [cited by applicant]
US 10384981B2 · Hall et al. · 2019 [cited by applicant]
US 10597335B2 · Dunn et al. · 2020 [cited by applicant]
US 10774008B2 · Subramanian et al. · 2020 [cited by applicant]
US 10774648B2 · Roberts et al. · 2020 [cited by applicant]
US 11027529B2 · Nelson et al. · 2021 [cited by applicant]
US 11034106B2 · Mega et al. · 2021 [cited by applicant]
US 20060006212A1 · Thebault et al. · 2006 [cited by applicant]
US 20060188736A1 · Luthra et al. · 2006 [cited by applicant]
US 20190084892A1 · Subramanian · 2019 [cited by examiner]
US 20190376389A1 · Roberts et al. · 2019 [cited by applicant]
US 20200189143A1 · Brandt et al. · 2020 [cited by applicant]
US 20200199028A1 · Dunn et al. · 2020 [cited by applicant]
Marchais et al., Capillary Infiltration of Hexadecane in Packed SiC Powder and in SiC/SiC Preforms: Pore Description and Calculation of Molten Si Infiltration, Ceramics International, vol. 42, 2016, pp. 7774-7780. [cited by applicant]